Brush Manufacturing: From Powder Mix to Finished Brush
Quick Answer
Electric motor brushes are manufactured by powder metallurgy. Carbon or graphite filler is milled and mixed with a pitch or resin binder, then pressed in a steel die. The compact is baked to cure or carbonise the binder, graphitised when required by the grade, and diamond machined to about plus or minus 0.05 mm. A copper shunt is then attached, often by staking. Baking affects the finished brush’s resistivity and bedding behaviour.
- The Short Answer: Pressed, Not Carved
- What Actually Goes Into a Brush
- Step 1: Milling and Mixing
- Step 2: Pressing to Near-Net Shape
- Step 3: Baking, Which Decides Almost Everything
- Step 4: Graphitisation for Electrographite Grades
- Step 5: Diamond Machining to Tolerance
- Step 6: The Shunt and the Top Plate
- What Is Measured Before a Brush Ships
- Why Cutting a Block of Carbon Does Not Work
- What a Brush Order Has to State
- When the Right Answer Is No Brushes At All
- References
- FAQ
The Short Answer: Pressed, Not Carved
A carbon brush can look like a small block of charcoal, but manufacturers form it from powder. They press the filler and binder in a die, then use baking and later processing to develop the structure and properties required in service.
Brush production involves six main steps. Omitting a step can change the part’s mechanical or electrical performance:
| Step | What happens | Key parameter | What goes wrong if it is skipped |
|---|---|---|---|
| 1 Mixing | filler milled and blended with binder | particle size and binder ratio | density varies from brush to brush |
| 2 Pressing | powder compacted in a steel die | 100 to 300 MPa | laminations and weak edges |
| 3 Baking | binder carbonised or cured | 150 to 1,200 degrees C depending on bond | crumbly body, wrong resistivity |
| 4 Graphitising | carbon converted to graphite lattice | 2,500 to 3,000 degrees C | high friction and contact drop |
| 5 Machining | diamond cutting to final size | about plus or minus 0.05 mm | brush cocks in the holder |
| 6 Assembly | shunt, top plate, spring | pull-off force | open circuit after a few hundred hours |
What motor brushes are explains their role, commutation and grade selection. Brushed DC motors describes the machines that use them. This article focuses on brush manufacturing.
What Actually Goes Into a Brush
The brush grade determines the material mix before manufacturing begins. The filler affects conductivity and friction, while the binder holds the compact together and changes during baking. Adding metal powder also changes the electrical properties.
| Grade family | Composition | Resistivity, order of magnitude | Working current density | Where it is used |
|---|---|---|---|---|
| Carbon-graphite | carbon black or coke with graphite, pitch or resin bond | tens of micro-ohm metres | 8 to 12 A/cm² | general industrial DC machines, power tools |
| Electrographite | same fillers, graphitised after baking | around 10 micro-ohm metres | 10 to 15 A/cm² | traction, high-speed and high-current duty |
| Natural graphite | natural graphite with resin bond | tens of micro-ohm metres, low friction | 5 to 10 A/cm² | slip rings, low-friction instrumentation duty |
| Metal-graphite | 30 to 80 percent copper with graphite | tenths of a micro-ohm metre | 20 to 30 A/cm² | starters, low-voltage high-current motors |
| Silver-graphite | silver with graphite | lowest of all, silver-dominated | signal level | precision slip rings and low-voltage signals |
These values are order-of-magnitude guides; the grade datasheet should be used for a specification. Resistivity may be reported in micro-ohm metres or micro-ohm centimetres. One micro-ohm metre equals 100 micro-ohm centimetres, so check the units when comparing datasheets.
Brush count and arrangement depend on the motor’s winding and commutation design. The relation between pole count and motor design is discussed in number of poles in a motor; confirm the required brush-arm arrangement from the machine drawing.

Step 1: Milling and Mixing
The filler arrives as coke, graphite or carbon black in lumps or coarse powder and is milled to a defined particle size distribution, typically with a median around ten to fifty micrometres. Particle-size distribution affects how consistently the powder packs in the die; the median alone does not describe the full mix.
Binder is then blended in. Pitch is mixed hot so that it coats the particles; resin is usually blended dry or in a solvent and dried back. Binder-to-filler ratio is one factor that affects porosity after baking, as the binder leaves pores while converting to carbon.
Metal-graphite grades are different again. Copper or silver powder is blended with the graphite at high loadings, and the mix has to be kept free of oxidation before pressing, because an oxidised copper particle becomes a high-resistance joint inside the brush.
Step 2: Pressing to Near-Net Shape
The mix is loaded into a hardened steel die and pressed uniaxially, usually between 100 and 300 MPa, to a shape that is already close to the finished brush. Some resin-bonded grades are warm-pressed at around 120 to 150 degrees C, which lets the binder flow and reduces the risk of laminations.
Pressing establishes the compact’s density distribution and green strength, meaning its strength before baking. Powder displacement can create a density gradient between the punch and die wall; an uneven fill may contribute to uneven wear. If the compact has insufficient green strength, it can crumble before reaching the furnace.
Pressing is also where the shunt hole or the shunt itself is often placed. Moulding the shunt in during pressing gives the strongest joint, but it constrains the die design and is normally reserved for high-volume grades.
Step 3: Baking, Which Decides Almost Everything
Baking develops the binder structure in the pressed compact. The temperature and atmosphere depend on the binder, so resin and pitch processes require different cycles.
Resin bond versus pitch bond
| Property | Resin-bonded | Pitch-bonded, baked |
|---|---|---|
| Treatment temperature | about 150 to 200 degrees C | about 800 to 1,200 degrees C |
| What the binder does | cross-links into a thermoset network | carbonises into a continuous carbon skeleton |
| Atmosphere | air or inert, with a controlled ramp | protective, to prevent oxidation of the carbon |
| Cycle length | hours | days, including heating and cooling ramps |
| Resulting character | harder, higher resistivity, lower current | better conductivity and strength, higher current |
The ramp is as important as the soak. Heat a pitch-bonded compact too quickly and the volatiles leave faster than the structure can accommodate, which opens cracks that only appear after machining. The same logic applies on the way down: cooling too fast leaves thermal stress in a brittle body.
This is the step a workshop cannot reproduce. A kitchen oven can cure a resin, but it cannot carbonise a pitch binder in a protective atmosphere over a multi-day cycle, and no amount of sanding afterwards substitutes for it.
Step 4: Graphitisation for Electrographite Grades
Electrographite grades go one furnace further. After baking, the parts are packed in a graphite-resistance furnace and taken to roughly 2,500 to 3,000 degrees C. At that temperature the turbostratic carbon formed during baking rearranges into a graphite lattice.
Graphite’s layered crystal structure can lower electrical resistivity and friction. Electrographite grades are therefore used in some traction applications that require higher current density; actual brush-face temperature depends on the complete operating conditions.
Not every grade goes through it, and the choice is not about quality. A natural-graphite brush already contains graphite and needs no conversion. A metal-graphite brush would be ruined by the temperature, because the copper would melt and coalesce.
Step 5: Diamond Machining to Tolerance
After firing, the brush is close to size but not to tolerance. It is machined with diamond tooling, because the material is abrasive enough to destroy carbide in a shift. Thickness is usually held to about plus or minus 0.05 mm, and the brush-to-holder clearance is set deliberately, often between 0.1 and 0.3 mm.
The clearance is specified to let the brush move as it heats. If it is too small, the brush can bind; if it is too large, it can chatter, arc and wear the commutator unevenly. Hand sanding does not reliably hold this fit, so the result can vary between parts.
Surface finish on the contact face matters for the first few hours only. What matters permanently is squareness: a brush whose face is not perpendicular to the shunt axis will run on one edge, and the resulting current concentration is what burns a commutator bar.
Step 6: The Shunt and the Top Plate
The shunt is the copper braid that carries current from the terminal to the brush body. Its attachment needs to withstand the motor’s temperature, vibration and current; a failed joint can interrupt operation and damage the commutator.
| Method | How it works | Strength | Typical use |
|---|---|---|---|
| Staking or crimping | braid forced into a tapered hole and swaged | high, mechanical | general industrial brushes |
| Ultrasonic welding | solid-state bond between copper and carbon | high, low contact resistance | high-current and traction grades |
| Moulded in during pressing | shunt embedded in the compact | highest | high-volume small motors |
| Soldering | tin-lead or lead-free solder | low | not appropriate, see below |
Why solder is not used
Heat from the brush face travels along the shunt toward the joint. Depending on the solder alloy and operating temperature, a soldered connection can soften or degrade under heavy brush duty. A failing joint may first cause intermittent contact, sparking or electrical interference before it opens completely. Confirm the joint method against the brush’s rated conditions.
The joint can be tested by applying a specified pull-off force to the shunt. Visual inspection alone may miss a weak attachment, so the release limit should come from the applicable grade or product specification.

What Is Measured Before a Brush Ships
Appearance alone does not confirm a brush’s electrical or mechanical properties. Production checks should follow the product specification. The table lists measurements that may be used; acceptance limits depend on the grade.
| Measurement | Method | What it predicts in service |
|---|---|---|
| Apparent density | mass over geometric volume | porosity, and therefore bedding and wear rate |
| Resistivity | four-point or clamped contact | contact drop and heating at the brush face |
| Hardness | Shore or Brinell-type indenter | wear against the commutator film |
| Transverse strength | three-point bend on a bar | resistance to chipping at the holder edge |
| Ash content | burn-off | abrasive inclusions that cut the commutator |
| Dimensions | micrometer and go/no-go gauges | fit in the holder, and freedom from chatter |
| Shunt pull-off | tensile pull on the braid | open circuit and intermittent faults |
The measurement that predicts field failure
The shunt pull-off test checks whether the attachment meets its specified strength. If a motor fails while the brushes still have substantial material remaining, inspect the shunt and its joint along with the other electrical and mechanical causes. The claim that this test identifies more field failures than electrical checks needs service data to support it.
The wider set of failure modes, including bedding, spring pressure and sparking limits, is covered in the brush reference page; this article deliberately does not repeat it.
Why Cutting a Block of Carbon Does Not Work
Cutting a block of carbon to size may produce a part that fits and runs briefly, but it does not reproduce the properties or tolerances of a manufactured brush. The differences include:
What a sawn block gets wrong
- The microstructure differs. Baking changes the binder and creates the structure and porosity needed for the specified brush grade; a sawn block does not reproduce that process.
- The resistivity may differ. If the material has not undergone the required carbonisation, contact drop and heating may be outside the brush’s intended range.
- The fit is difficult to control. The article cites a machining tolerance of plus or minus 0.05 mm; hand sanding may not hold that tolerance, and excess clearance can cause chatter or arcing.
- The shunt joint may not withstand operating conditions. Soldered or glued joints should not be assumed suitable without confirming the material, temperature rating and attachment specification.
Machining graphite also creates conductive dust. Use suitable dust extraction and housekeeping controls to limit contamination of open motors and electrical equipment.
What a Brush Order Has to State
Brush selection depends on a complete specification. These six items help the supplier match the brush to the motor and its operating conditions:
- Dimensions and tolerance, including the thickness tolerance and the corner radii, not just the nominal block size.
- Grade and grade source, because two suppliers’ grades with the same name are not the same recipe.
- Shunt length, gauge and terminal, with the pull-off force required.
- Spring pressure the machine applies, since the grade has to be matched to it.
- Current density and duty, in A/cm² and in hours per day.
- Environment, including humidity, oil mist and whether the machine is washed down, because ingress is what kills brush gear.
Environmental conditions affect the motor’s ingress protection and brush-gear enclosure; retrofit requirements should specify both. Motor efficiency classes are described in motor efficiency class. Current density in A/cm² should be considered alongside shaft load and duty. The calculation method is covered in calculating motor torque.
When the Right Answer Is No Brushes At All
We manufacture brushless motors and also supply brushed units, so we have a commercial interest in the choice discussed here. A machine that needs new brushes every few hundred hours may have an underlying issue with commutation, spring pressure, loading or operating conditions. Check those causes before changing motor type.
Brush life is commonly cited as 1,000 to 3,000 hours, although actual life varies with motor design and duty. The commutator may also need machining after several brush replacements, depending on wear. A brushless motor removes the brush and commutator wear surfaces and can recover braking energy when the drive and application support regeneration.
What replaces the commutator
Commutation moves from a mechanical contact to an electronic one. A three-phase inverter switches the winding according to rotor position, with the position coming from Hall sensors or from a sensorless estimator, a choice set out in Hall sensor versus sensorless commutation. The magnetic circuit that makes this work is described in how a BLDC motor works.
Brushless motors require an electronic controller, but they do not use a brush holder, commutator or brush-service interval. Their efficiency relative to a brushed motor depends on the designs and load point; compare the complete motor-and-controller system under the intended duty. The comparison for one product category is worked through in BLDC versus brushed DC for micro pumps, and the general case in BLDC versus brushed DC motors.
Vehicle applications make the brushless-versus-brushed trade-off at production scale; an example is discussed in BLDC versus DC motors for electric vehicles. For applications where torque is the main requirement, see the high-torque BLDC guide.
Chasing brush life on a small motor? Send the duty cycle in hours, the load torque at the shaft, the supply voltage and the envelope you have. We will tell you whether the brush is the right wear part or whether the topology should change. Contact the engineering team.
References
- International Electrotechnical Commission. (2022). IEC 60034-1:2022 Rotating electrical machines – Part 1: Rating and performance. webstore.iec.ch/en/publication/65446
- International Electrotechnical Commission. (2014). IEC 60034-2-1:2014 Rotating electrical machines – Part 2-1: Standard methods for determining losses and efficiency from tests. webstore.iec.ch/en/publication/121
- International Electrotechnical Commission. (2018). IEC 60034-14:2018 Rotating electrical machines – Part 14: Mechanical vibration of certain machines with shaft heights 56 mm and higher. webstore.iec.ch/en/publication/59889
- International Electrotechnical Commission. (2013). IEC 60529:1989+AMD1:1999+AMD2:2013 Degrees of protection provided by enclosures (IP Code). webstore.iec.ch/en/publication/2452
- International Electrotechnical Commission. (2023). IEC 61800-9-2:2023 Adjustable speed electrical power drive systems – Ecodesign for power drive systems, motor starters, power electronics and their driven applications. webstore.iec.ch/en/publication/111276
- National Electrical Manufacturers Association. (2024). NEMA standards for motors and generators. nema.org/standards
- European Parliament and Council. (2011). Directive 2011/65/EU on the restriction of the use of certain hazardous substances in electrical and electronic equipment (RoHS). eur-lex.europa.eu/eli/dir/2011/65/oj
- European Parliament and Council. (2006). Regulation (EC) No 1907/2006 concerning the Registration, Evaluation, Authorisation and Restriction of Chemicals (REACH). eur-lex.europa.eu/eli/reg/1907/2006/oj
- European Commission. (2019). Commission Regulation (EU) 2019/1781 laying down ecodesign requirements for electric motors and variable speed drives. eur-lex.europa.eu/eli/reg/2019/1781/oj
- U.S. Department of Energy. (2024). Motors and drives systems – advanced manufacturing office resources. energy.gov/eere/amo/motor-systems
FAQ
Q: How are electric motor brushes made?
They are made by powder metallurgy. Carbon or graphite filler is milled and mixed with a pitch or resin binder, pressed in a steel die to a near-net shape, baked to carbonise the binder, graphitised if the grade requires it, then diamond machined to final size and fitted with a copper shunt. Nothing is carved from a solid block of carbon.
Q: Why can’t I cut a brush from a block of carbon?
Material composition affects brush performance, and baking changes the binder into a carbon structure with controlled porosity. A sawn block has not undergone that process, so its resistivity, bedding behaviour and fit may differ from the specified brush. The article cites a tolerance of plus or minus 0.05 mm; confirm the required value for the specific holder.
Q: What temperature are motor brushes baked at?
It depends on the binder. Resin-bonded grades are cured around 150 to 200 degrees C. Pitch-bonded grades are fired to roughly 800 to 1,200 degrees C in a protective atmosphere to carbonise the binder. Electrographite grades then go through graphitisation at about 2,500 to 3,000 degrees C, which rearranges the carbon into a graphite lattice.
Q: How is the shunt attached to a brush?
The shunt may be staked, crimped or ultrasonically welded into the brush body, or embedded during pressing. Solder is generally unsuitable for high-temperature brush duty unless the joint is specifically rated for the operating conditions. The shunt pull-off force should be included in the release specification.
Q: What is graphitisation and which brushes need it?
It is a high-temperature treatment that converts amorphous carbon into a graphite crystal structure, which lowers resistivity and friction. Only electrographite grades go through it. Carbon-graphite, natural graphite, metal-graphite and silver-graphite grades do not, and each is chosen for a different combination of current density, contact drop and wear.
Q: Is it worth making brushes instead of buying them?
Making brushes in-house is rarely economical at low volume because production requires suitable tooling, furnace cycles and release testing. The grade must also match the commutator, spring pressure and duty. If brushes fail repeatedly, diagnose the cause first; changing the motor topology may be an option, but its cost and performance should be compared with a suitable replacement brush.